| Availability: | |
|---|---|
Printing Parameters
| Description | Data | Desciption | Data | 
| Nozzle Temperature | 190—230℃ | Heated bed Temperature | 50-60℃ | 
| Printing Platform Material | Soft Magnetic Sticker | Printing Platform Surface Treatment | No Processing Required | 
| Bottom Value Sparation Distance | 0.4-0.6 | Withdrawal Distance | 1mm | 
| Environment Temperature | Room temperature | Withdrawal Speed | 50mm/s | 
| Recommended Support Material | PVA | Drying Temperature | 50℃ | 
| Printing Speed | 40--250 mm/s | Cooling Fan | 100% | 
| Suitable for all FDM 3D Printers / 3D Printing Machines | |||
Physical Properties
| Properties | Testing method | Value | 
| Density | ASTM D792 | @23℃ 1.25g/cm3 | 
| Melt Flow Index | ASTM D1238 | 190℃/2.16kg 9g/10min | 
Flame Properties
| Properties | Testing method | Value | 
| Flame Retardance | UL94 | @1.5mm HB | 
Thermal Performance
| Properties | Testing Method | Value | |
| Glass Transsition | ASTM D7426 | @10℃/min 60.9℃ | |
| Melting Temperature | ASTM D7426 | @10℃/min 164℃ | |
| Decomposition Temperature | ASTM E2402 | @20℃/min ≥364℃ | |
| Cofficient of Thermal Expansion | ASTM E831 | 101×10-06 ㎛(m· ℃) | |
| Shrinking Percentage | ASTM D955 | @23℃ 0.1-0.3% | |
| Vicat Softening Temperature | ASTM D1525 | 5kg,50℃/h 54℃ | |
| Heat Distortion Temperature | ASTM D648 | 0.45Mpa/53℃ | |
Mechanical Performance
| Printing Direction | Testing Standard | Data | 
| Tensile Strength | ASTM D638 | @50mm/min 60.6Mpa | 
| Elongation at break | ASTM D638 | @50mm/min 6.3% | 
| Flexural Strength | ASTM D790 | @2mm/min 65Mpa | 
| Flexural Modulus | ASTM D790 | @2mm/min 1895Mpa | 
| Charpy Impact Strength with Notched | ASTM D256 | @3.2mm 33J/㎡ | 
| Young Modulus | ASTM D638 | @1mm/min 2760Mpa | 
Chemical Resistance
| Item | Grade | 
| Weak Acids Affect pH3-6 | Good | 
| Strong Acids Affect pH<3 | Poor | 
| Weak Base Affect pH8-10 | Good | 
| Strong Base Affect pH>10 | Poor | 
| Deionized Water | Good | 
| Athyl Alcohol | Average | 
| Acetone | Poor | 
| Gasoline | Good | 
| Ether | Good | 
Printing Parameters
| Description | Data | Desciption | Data | 
| Nozzle Temperature | 190—230℃ | Heated bed Temperature | 50-60℃ | 
| Printing Platform Material | Soft Magnetic Sticker | Printing Platform Surface Treatment | No Processing Required | 
| Bottom Value Sparation Distance | 0.4-0.6 | Withdrawal Distance | 1mm | 
| Environment Temperature | Room temperature | Withdrawal Speed | 50mm/s | 
| Recommended Support Material | PVA | Drying Temperature | 50℃ | 
| Printing Speed | 40--250 mm/s | Cooling Fan | 100% | 
| Suitable for all FDM 3D Printers / 3D Printing Machines | |||
Physical Properties
| Properties | Testing method | Value | 
| Density | ASTM D792 | @23℃ 1.25g/cm3 | 
| Melt Flow Index | ASTM D1238 | 190℃/2.16kg 9g/10min | 
Flame Properties
| Properties | Testing method | Value | 
| Flame Retardance | UL94 | @1.5mm HB | 
Thermal Performance
| Properties | Testing Method | Value | |
| Glass Transsition | ASTM D7426 | @10℃/min 60.9℃ | |
| Melting Temperature | ASTM D7426 | @10℃/min 164℃ | |
| Decomposition Temperature | ASTM E2402 | @20℃/min ≥364℃ | |
| Cofficient of Thermal Expansion | ASTM E831 | 101×10-06 ㎛(m· ℃) | |
| Shrinking Percentage | ASTM D955 | @23℃ 0.1-0.3% | |
| Vicat Softening Temperature | ASTM D1525 | 5kg,50℃/h 54℃ | |
| Heat Distortion Temperature | ASTM D648 | 0.45Mpa/53℃ | |
Mechanical Performance
| Printing Direction | Testing Standard | Data | 
| Tensile Strength | ASTM D638 | @50mm/min 60.6Mpa | 
| Elongation at break | ASTM D638 | @50mm/min 6.3% | 
| Flexural Strength | ASTM D790 | @2mm/min 65Mpa | 
| Flexural Modulus | ASTM D790 | @2mm/min 1895Mpa | 
| Charpy Impact Strength with Notched | ASTM D256 | @3.2mm 33J/㎡ | 
| Young Modulus | ASTM D638 | @1mm/min 2760Mpa | 
Chemical Resistance
| Item | Grade | 
| Weak Acids Affect pH3-6 | Good | 
| Strong Acids Affect pH<3 | Poor | 
| Weak Base Affect pH8-10 | Good | 
| Strong Base Affect pH>10 | Poor | 
| Deionized Water | Good | 
| Athyl Alcohol | Average | 
| Acetone | Poor | 
| Gasoline | Good | 
| Ether | Good | 
Mechanical Properties
| Property | Testing Method | Testing Condition | Injection Molding Typical Value | 3D Printing X-Y Axis Typical Value | 3D Printing Z Axis Typical Value | Unit | 
| Tensile Strength | ISO 527 | 50mm/min | 52.5 | 45.2 ± 4 | 37.6 ± 4 | MPa | 
| Elongation at Break | ISO 527 | 50mm/min | 66.7 | 11.4 ± 1.8 | 1.7 ± 0.5 | % | 
| Tensile Modulus | ISO 527 | 50mm/min | 1668 | 1720 ± 100 | 1711 ± 100 | MPa | 
| Flexural Strength | ISO 178 | 2mm/min | 76.2 | 68.7 ± 6.5 | 61.8 ± 6.5 | MPa | 
| Flexural Modulus | ISO 178 | 2mm/min | 2280 | 1967 ± 100 | 1901 ± 100 | MPa | 
| Charpy Impact Strength | ISO 179 | 23℃ | NB | 25 ± 3.5 | 10.5 ± 2 | KJ/m² | 
| Izod Impact Strength | ISO 180 | 23℃ | NB | 29.8 ± 3.5 | 7.7 ± 2 | KJ/m² | 
Physical Properties
| Property | Testing Method | Testing Condition | Typical Value | Unit | 
| Density | ISO 1183 | Immersion | 1.26 | g/cm3 | 
| Melt Flow index(MFR) | ISO 1133 | 240℃ 2.16kg | 10.0 | g/10 min | 
Moisture Absorption
| Property | Testing Method | Testing Condition | Injection Molding Typical Value | 3D Printing Typical Value | Unit | 
| Moisture Absorption | ISO 62 | 50%RH*23℃ | 0.06 | 0.05 | % | 
Chemical Properties
| Property | Testing Result | 
| Weak Acid Resistance | Not Resistant | 
| Strong Acid Resistance | Not Resistant | 
| Weak Base Resistance | Not Resistant | 
| Strong Base Resistance | Not Resistant | 
| Organic Solution Resistance | Not Resistant | 
Thermal Properties
| Property | Testing Method | Testing Condition | Injection Molding Typical Value | 3D Printing X-Y Axis Typical Value | 3D Printing Z Axis Typical Value | Unit | 
| Glass Transition Temperature | DSC | 10℃/min | 81.6 | ℃ | ||
| Decomposition Temperature | TGA | 20℃/min | 387.5 | ℃ | ||
| Heat Distortion Temperature | ISO 75 | 0.45MPa | 71.8 | 74.8 | 72.9 | ℃ | 
| Heat Distortion Temperature | ISO 75 | 1.8MPa | 63.8 | 69.8 | 67.6 | ℃ | 
| Vicat Softening Temperature | ISO 306 | 50℃/10N | 79.7 | 78.0 | 77.3 | ℃ | 
Recommended 3D Printing Parameters
*Based on 0.4 mm nozzle. Printing conditions may vary with different nozzle diameters
| Printing Temperature | 240 – 260 (℃) | 
| Bed Temperature | 70 - 80 (℃) | 
| Wall Layers | 2 Layers | 
| Top and Bottom Layers | 4 Layers | 
| Infill | 100% | 
| Ambient Temperature | 25℃ | 
| Cooling Fan | 0 - 10% | 
| Printing Speed | 30 – 50 (mm/s) | 
| Nozzle Diameter | 0.4 mm | 
3DPrinting Actual Parameters
*All specimens must be left at room temperature for 24 hours before testing. The parameters are based on the Bambulab PES 3D printer.
| Printing Temperature | 250 (℃) | 
| Bed Temperature | 80 (℃) | 
| Wall Layers | 2 Layers | 
| Top and Bottom Layers | 4 Layers | 
| Infill | 100% | 
| Ambient Temperature | 25℃ | 
| Cooling Fan | 10% | 
| Printing Speed | 50 (mm/s) | 
| Nozzle Diameter | 0.4 mm | 
Mechanical Properties
| Property | Testing Method | Testing Condition | Injection Molding Typical Value | 3D Printing X-Y Axis Typical Value | 3D Printing Z Axis Typical Value | Unit | 
| Tensile Strength | ISO 527 | 50mm/min | 52.5 | 45.2 ± 4 | 37.6 ± 4 | MPa | 
| Elongation at Break | ISO 527 | 50mm/min | 66.7 | 11.4 ± 1.8 | 1.7 ± 0.5 | % | 
| Tensile Modulus | ISO 527 | 50mm/min | 1668 | 1720 ± 100 | 1711 ± 100 | MPa | 
| Flexural Strength | ISO 178 | 2mm/min | 76.2 | 68.7 ± 6.5 | 61.8 ± 6.5 | MPa | 
| Flexural Modulus | ISO 178 | 2mm/min | 2280 | 1967 ± 100 | 1901 ± 100 | MPa | 
| Charpy Impact Strength | ISO 179 | 23℃ | NB | 25 ± 3.5 | 10.5 ± 2 | KJ/m² | 
| Izod Impact Strength | ISO 180 | 23℃ | NB | 29.8 ± 3.5 | 7.7 ± 2 | KJ/m² | 
Physical Properties
| Property | Testing Method | Testing Condition | Typical Value | Unit | 
| Density | ISO 1183 | Immersion | 1.26 | g/cm3 | 
| Melt Flow index(MFR) | ISO 1133 | 240℃ 2.16kg | 10.0 | g/10 min | 
Moisture Absorption
| Property | Testing Method | Testing Condition | Injection Molding Typical Value | 3D Printing Typical Value | Unit | 
| Moisture Absorption | ISO 62 | 50%RH*23℃ | 0.06 | 0.05 | % | 
Chemical Properties
| Property | Testing Result | 
| Weak Acid Resistance | Not Resistant | 
| Strong Acid Resistance | Not Resistant | 
| Weak Base Resistance | Not Resistant | 
| Strong Base Resistance | Not Resistant | 
| Organic Solution Resistance | Not Resistant | 
Thermal Properties
| Property | Testing Method | Testing Condition | Injection Molding Typical Value | 3D Printing X-Y Axis Typical Value | 3D Printing Z Axis Typical Value | Unit | 
| Glass Transition Temperature | DSC | 10℃/min | 81.6 | ℃ | ||
| Decomposition Temperature | TGA | 20℃/min | 387.5 | ℃ | ||
| Heat Distortion Temperature | ISO 75 | 0.45MPa | 71.8 | 74.8 | 72.9 | ℃ | 
| Heat Distortion Temperature | ISO 75 | 1.8MPa | 63.8 | 69.8 | 67.6 | ℃ | 
| Vicat Softening Temperature | ISO 306 | 50℃/10N | 79.7 | 78.0 | 77.3 | ℃ | 
Recommended 3D Printing Parameters
*Based on 0.4 mm nozzle. Printing conditions may vary with different nozzle diameters
| Printing Temperature | 240 – 260 (℃) | 
| Bed Temperature | 70 - 80 (℃) | 
| Wall Layers | 2 Layers | 
| Top and Bottom Layers | 4 Layers | 
| Infill | 100% | 
| Ambient Temperature | 25℃ | 
| Cooling Fan | 0 - 10% | 
| Printing Speed | 30 – 50 (mm/s) | 
| Nozzle Diameter | 0.4 mm | 
3DPrinting Actual Parameters
*All specimens must be left at room temperature for 24 hours before testing. The parameters are based on the Bambulab PES 3D printer.
| Printing Temperature | 250 (℃) | 
| Bed Temperature | 80 (℃) | 
| Wall Layers | 2 Layers | 
| Top and Bottom Layers | 4 Layers | 
| Infill | 100% | 
| Ambient Temperature | 25℃ | 
| Cooling Fan | 10% | 
| Printing Speed | 50 (mm/s) | 
| Nozzle Diameter | 0.4 mm |